Vergleich von thermoplastischen Polyurethan-Werkstoffen

 

 


  

 

  Polyurethane
(Ether Based)

  Polyurethane
(Ether Based)

 Polyurethane
(Ether Based)

  Polyurethane
(Ether Based)

 Polyurethane
(Ester Based)

  Polyurethane
(Ester Based)

 

Shore Value for Hardness

(ASTM D-2240)

 85A

 90A

50D

55D

90A

50D

 

Specific Gravity

(ASTM D-792)

 1.12

1.13

1.16

1.16

1.21

1.23

 

Ultimate (Psi)

Tensile Strength

(ASTM D-412)

 5200

5400

8700

8400

8000

7350

 

Ultimate Elongation (%)

(ASTM D-412)

 530

460

410

410

450

510

 

Tear Strength

Die “C” (PLi)

(ASTM D-624)

 630

730

810

810

600

930

 

Taber Abrasion Resistance

(ASTM D-1044)

 30mg

 

45mg        

 

 

2.0 mg / 1000 cycles  (CS-17)

ASTM D-3389

 

3.5 mg / 1000 cycles  (CS-17)

ASTM D-3389

 

2.6 mg / 1000 cycles  (CS-17)

ASTM D-1044

 

 

2.5 mg / 1000 cycles  (CS-17)

ASTM D-1044

 

Vicat Softening Temperature (°C)

(ASTM D-1044)

 100

120

129

129

92

131

 

Glass Transition Temperature

(DSC), °C

 -38

-35

-33

-36

-3

-22

 

 Note:

    • Die oben angegebenen Werte sind Durchschnittswerte und gelten nicht als Spezifikationen verstanden werden.